Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® T7300EG10 LS BK23346 - PA*-GF50 - BASF

Material Data Center offers the following functions for Ultramid® T7300EG10 LS BK23346:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid T datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit
Glass-fiber reinforced, heat aging resistant injection molding grade with excellent surface quality based on semi-crystalline polyamides with partially aromatic content. The product can be characterized as compound with very high strength and stiffness even after moisture uptake.

Markets & applications
Automotive: structural parts, metal replacement, brake parts, interior, powertrain
E&E: electrical appliances, cell phones
Consumer goods: home appliances, consumer electronics, furniture fittings
Caractéristiques des transformations/physiquessec / condUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 7 / * cm³/10min ISO 1133
Température 275 / * °C -
Charge 5 / * kg -
Retrait au moulage, parallèle 0.5 / * % ISO 294-4, 2577
Retrait au moulage, perpendiculaire 0.7 / * % ISO 294-4, 2577
Propriétés mécaniquessec / condUnitéNorme du test
ISO Data
Module en traction 17700 / 16600 MPa ISO 527
Contrainte à la rupture 255 / 210 MPa ISO 527
Déformation à la rupture 2.8 / 3 % ISO 527
Résistance au choc Charpy, +23°C 108 / 100 kJ/m² ISO 179/1eU
Résistance au choc Charpy, -30°C 90 / 88 kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 15 / 15 kJ/m² ISO 179/1eA
Résistance au choc Charpy (entaillé), -30°C 14 / 14 kJ/m² ISO 179/1eA
Propriétés thermiquessec / condUnitéNorme du test
ISO Data
Température de fusion, 10°C/min 255 / * °C ISO 11357-1/-3
Température de fléchissement s/chrg, 1.80 MPa 240 / * °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 255 / * °C ISO 75-1/-2
Propriétés diversessec / condUnitéNorme du test
Absorption d'humidité 1.2 / * % Sim. to ISO 62
Masse volumique 1600 / - kg/m³ ISO 1183
Propriétés spécifiques à la matièresec / condUnitéNorme du test
ISO Data
Indice de viscosité 134 / * cm³/g ISO 307, 1157, 1628
Préparation et conditionnement des éprouvettesValeurUnitéNorme du test
ISO Data
Injection, température de la matière fondue 310 °C ISO 294
Injection, température du moule 100 °C ISO 294
Injection, vitesse d'injection 200 mm/s ISO 294
Recommandations pour la transformation Moulage par injectionValeurUnitéNorme du test
Pré-séchage - température 110 °C -
Pré-séchage - temps 8 h -
L'humidité de traitement ≤0.15 % -
Température de la matière fondue 300 - 320 °C -
Température du moule 80 - 120 °C -
Temps de sejour maximum 5 min -
Fonctions
Viscosité / Vitesse de cisaillement , Ultramid® T7300EG10 LS BK23346, PA*-GF50, BASF
Contrainte de cisaillement / Vit. de cisaillement , Ultramid® T7300EG10 LS BK23346, PA*-GF50, BASF
Contrainte / Déformation , Ultramid® T7300EG10 LS BK23346 (sec), PA*-GF50, BASF
Contrainte / Déformation , Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Module sécant / Déformation , Ultramid® T7300EG10 LS BK23346 (sec), PA*-GF50, BASF
Module sécant / Déformation , Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Contrainte / Déformation (isochrone) 23°C, Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Module de fluage / Temps 23°C, Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Courbe de fluage 23°C, Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Contrainte / Déformation (isochrone) 80°C, Ultramid® T7300EG10 LS BK23346 (sec), PA*-GF50, BASF
Module de fluage / Temps 80°C, Ultramid® T7300EG10 LS BK23346 (sec), PA*-GF50, BASF
Courbe de fluage 80°C, Ultramid® T7300EG10 LS BK23346 (sec), PA*-GF50, BASF
Module de traction / Température , Ultramid® T7300EG10 LS BK23346 (sec), PA*-GF50, BASF
Module de traction / Température , Ultramid® T7300EG10 LS BK23346 (cond.), PA*-GF50, BASF
Caractéristiques
Transformation
Moulage par injection
Conditionnement
Granulés, Noir
Propriétés spéciales
Stabilisé à la chaleur
Caractéristiques
Marquage au laser
Applications
Automobile, Électrotechnique et électrique
Disponibilité régionale
Autres informations
Moulages par injection
PREPROCESSING
Pre/Post-processing, Pre-drying, Temperature: 110 °C
Pre/Post-processing, Pre-drying, Time: 8 h

PROCESSING
injection molding, Melt temperature, range: 280 - 310 °C
injection molding, Melt temperature, recommended: 300 °C
injection molding, Mold temperature, range: 80 - 120 °C
injection molding, Mold temperature, recommended: 100 °C
injection molding, Dwell time, thermoplastics: 5 min
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.